Hastelloy C-276 vs Hastelloy C-22
Hastelloy C-276 and C-22 are Haynes International nickel-chromium-molybdenum alloys, made to largely the same ASTM standards, and Aurico Alloys LLP supplies both as sheet, plate, foil and round bar. The difference is the balance between chromium and molybdenum: C-22 carries more chromium and less molybdenum than C-276. Chromium handles oxidising conditions and molybdenum reducing ones, so the choice follows the chemistry of the service.
How they differ
- Oxidising service. C-22 is the choice where the service is oxidising: ferric and cupric chlorides, nitric acid and mixed acids. Where hydrochloric acid carries ferric or cupric ions, Special Metals points to C-22.
- Reducing and mixed service. C-276 is the stronger choice in reducing conditions, and the grade specified when the service is mixed, cyclic or not fully characterised.
- Pitting and crevice attack. In oxidising chlorides, C-22 has outstanding resistance to pitting and crevice attack.
- Sulphuric acid. C-276 has useful resistance up to 10% sulphuric acid at boiling and at all concentrations to about 80 °C, though in dilute sulphuric acid Special Metals ranks Incoloy 825 ahead of it.
- Welding. Both hold carbon very low (see the composition table). C-276 can be welded without a post-weld solution anneal, and C-22 resists sensitisation in the weld heat-affected zone.
Where each is used
Hastelloy C-276
- Flue gas desulphurisation ducting and scrubbers
- Pulp and paper bleaching equipment
- Pickling lines and acid handling
- Waste treatment and incineration scrubbers
Hastelloy C-22
- Mixed and oxidising acid service
- Flue gas desulphurisation
- Pharmaceutical and agrichemical reactors
- Pickling and metal finishing plant
Designations and physical constants
| Property | Hastelloy C-276 | Hastelloy C-22 |
|---|---|---|
| UNS number | N10276 | N06022 |
| Werkstoff / EN number | 2.4819 | 2.4602 |
| EN name | NiMo16Cr15W | NiCr21Mo14W |
| Density | 8.89 g/cm3 | 8.69 g/cm3 |
| Melting range | 1323-1371 °C | 1357-1399 °C |
From the Haynes International data sheets for both grades. A dash means no such designation is published for the grade.
Chemical composition
| Element (%) | Hastelloy C-276 | Hastelloy C-22 |
|---|---|---|
| Nickel (Ni) | Balance | Balance |
| Chromium (Cr) | 14.5–16.5 | 20.0–22.5 |
| Molybdenum (Mo) | 15.0–17.0 | 12.5–14.5 |
| Iron (Fe) | 4.0–7.0 | 2.0–6.0 |
| Tungsten (W) | 3.0–4.5 | 2.5–3.5 |
| Cobalt (Co) | 2.5 max | 2.5 max |
| Manganese (Mn) | 1.0 max | 0.50 max |
| Vanadium (V) | 0.35 max | 0.35 max |
| Carbon (C) | 0.010 max | 0.015 max |
| Silicon (Si) | 0.08 max | 0.08 max |
| Phosphorus (P) | 0.04 max | 0.02 max |
| Sulfur (S) | 0.03 max | 0.02 max |
Specification limits from the Haynes International data sheets for both grades, not measured values for a lot; the mill test certificate supplied with an order states the actual analysis. A dash means the bulletin sets no limit for that element.
Standards by product form
| Product form | Hastelloy C-276 | Hastelloy C-22 |
|---|---|---|
| Plate, sheet and strip | ASTM B575 | ASTM B575 |
| Rod and bar | ASTM B574 / B564 | ASTM B574 / B564 |
| Pipe and tube | ASTM B619 / B622 / B626 | ASTM B619 / B622 |
| Fittings | ASTM B366 | ASTM B366 |
The standard is written for the product form: quote the one that matches the product you are ordering. A dash means no standard is published for the grade in that form.
Forms, sizes and certificates for each grade are on the Hastelloy C-276 and Hastelloy C-22 pages. How each behaves in sulphuric, hydrochloric, nitric and the other acids, against the other grades, is in our acid and alkali service guide.