Monel 400 vs Monel K-500
Monel K-500 is Monel 400's nickel-copper base with aluminium and titanium added. Both are Special Metals alloys. Age-hardening precipitates the aluminium and titanium as gamma prime, which lifts the strength of K-500 well above that of Monel 400 while keeping the corrosion resistance of the nickel-copper matrix. Aurico Alloys LLP supplies Monel 400 as round bar, sheet, plate, foil and wire, and Monel K-500 as round bar, sheet, plate and foil.
How they differ
- Strength. Monel 400 is not age-hardenable; its strength comes from cold work. Monel K-500 takes its strength from age-hardening, so it is chosen where a part needs strength as well as the corrosion resistance of the nickel-copper base.
- Corrosion. K-500 keeps the corrosion behaviour of Monel 400 on the same base, so seawater and caustic service carry across. Monel 400 is the nickel alloy most used in hydrofluoric acid and is nearly as resistant as Nickel 200 to caustic soda, but nitric acid above 0.5% attacks it rapidly.
- Weight. Monel 400 is the heavier of the two (densities below); the aluminium in K-500 is what makes the difference, and it matters when a drawing is costed by weight.
- Temperature and magnetism. Monel 400 is useful from sub-zero temperatures to about 480 °C, with no ductile-to-brittle transition on cooling. K-500 holds its properties down to sub-zero temperatures and stays non-magnetic.
- Standards. They are ordered to different standards in every form, so quote the one that matches the grade as well as the product; the table below gives each.
Where each is used
Monel 400
- Marine propeller and pump shafting, seawater piping and fittings
- Heat exchangers and condensers in brackish and salt water
- Hydrofluoric acid alkylation plant and HF handling equipment
- Valve trim, pump casings and fasteners for chemical service
Monel K-500
- Pump and propeller shafts in seawater service
- Doctor blades and scrapers
- Oil-field drill collars and downhole instrumentation
- Fasteners and springs needing strength with marine corrosion resistance
Designations and physical constants
| Property | Monel 400 | Monel K-500 |
|---|---|---|
| UNS number | N04400 | N05500 |
| Werkstoff / EN number | 2.4360 / 2.4361 | 2.4375 |
| Density | 8.80 g/cm3 | 8.44 g/cm3 |
| Melting range | 1300-1350 °C | 1315-1350 °C |
From the Special Metals data sheets for both grades. A dash means no such designation is published for the grade.
Chemical composition
| Element (%) | Monel 400 | Monel K-500 |
|---|---|---|
| Nickel (Ni) | 63.0 min | 63.0 min |
| Carbon (C) | 0.3 max | 0.25 max |
| Manganese (Mn) | 2.0 max | 1.5 max |
| Iron (Fe) | 2.5 max | 2.0 max |
| Sulfur (S) | 0.024 max | 0.01 max |
| Silicon (Si) | 0.5 max | 0.5 max |
| Copper (Cu) | 28.0–34.0 | 27.0–33.0 |
| Aluminium (Al) | — | 2.30–3.15 |
| Titanium (Ti) | — | 0.35–0.85 |
Specification limits from the Special Metals data sheets for both grades, not measured values for a lot; the mill test certificate supplied with an order states the actual analysis. A dash means the bulletin sets no limit for that element.
Standards by product form
| Product form | Monel 400 | Monel K-500 |
|---|---|---|
| Plate, sheet and strip | ASTM B127 / AMS 4544 | QQ-N-286 |
| Rod and bar | ASTM B164 / B564 | ASTM B865 |
| Wire | ASTM B164 / AMS 4730 / 4731 | QQ-N-286 / ISO 9724 |
| Pipe and tube | ASTM B163 / B165 | — |
| Fittings | ASTM B366 | — |
The standard is written for the product form: quote the one that matches the product you are ordering. A dash means no standard is published for the grade in that form.