Inconel 625 vs Inconel 718
Inconel 625 and Inconel 718 are both Special Metals nickel-chromium alloys, and Aurico Alloys LLP supplies both as sheet, plate, coil, round bar, wire, pipe, tube and fittings. They are chosen for different reasons. Special Metals attributes the strength of 625 to molybdenum and niobium stiffening its nickel-chromium matrix, so it needs no precipitation-hardening treatment. 718 is age-hardened: a heat treatment precipitates its niobium, titanium and aluminium and lifts it to far higher strength.
How they differ
- Strength. 625 is strong as annealed and as welded, and needs no ageing. 718 reaches far higher strength after its ageing treatment, which is why it is chosen where strength decides the grade.
- Corrosion. 625 carries about three times the molybdenum of 718, with more chromium and more nickel. That gives it corrosion resistance in both oxidising and reducing conditions, in seawater and in chlorides, and makes it the most widely specified grade of the family.
- Base metal. 625 is nickel-based, with iron held to a few per cent. 718 is nickel plus cobalt on an iron balance.
- Welding. 625 needs no ageing after welding. Special Metals describes the ageing response of 718 as sluggish, which lets it be annealed and welded without hardening as it heats and cools, and gives it outstanding resistance to post-weld cracking.
- Weight. 718 is the lighter of the two (densities below), which matters when a part is costed by weight.
Where each is used
Inconel 625
- Seawater and subsea hardware
- Chemical process piping and vessels
- Aerospace ducting and exhaust systems
- Flue gas desulphurisation and scrubbers
Inconel 718
- Gas turbine discs, blades and casings
- Rocket and aerospace structural parts
- Downhole and wellhead components
- High-strength fasteners and springs
Designations and physical constants
| Property | Inconel 625 | Inconel 718 |
|---|---|---|
| UNS number | N06625 | N07718 |
| Werkstoff / EN number | 2.4856 | 2.4668 |
| Density | 8.44 g/cm3 | 8.19 g/cm3 |
| Melting range | 1290-1350 °C | 1260-1336 °C |
From the Special Metals data sheets for both grades. A dash means no such designation is published for the grade.
Chemical composition
| Element (%) | Inconel 625 | Inconel 718 |
|---|---|---|
| Nickel (Ni) | 58.0 min | — |
| Chromium (Cr) | 20.0–23.0 | 17.0–21.0 |
| Iron (Fe) | 5.0 max | Balance |
| Molybdenum (Mo) | 8.0–10.0 | 2.80–3.30 |
| Niobium + Tantalum (Nb+Ta) | 3.15–4.15 | 4.75–5.50 |
| Carbon (C) | 0.10 max | 0.08 max |
| Manganese (Mn) | 0.50 max | 0.35 max |
| Silicon (Si) | 0.50 max | 0.35 max |
| Phosphorus (P) | 0.015 max | 0.015 max |
| Sulfur (S) | 0.015 max | 0.015 max |
| Aluminium (Al) | 0.40 max | 0.20–0.80 |
| Titanium (Ti) | 0.40 max | 0.65–1.15 |
| Cobalt (Co) | 1.0 max (if determined) | 1.0 max |
| Nickel + Cobalt (Ni+Co) | — | 50.0–55.0 |
| Copper (Cu) | — | 0.30 max |
| Boron (B) | — | 0.006 max |
Specification limits from the Special Metals data sheets for both grades, not measured values for a lot; the mill test certificate supplied with an order states the actual analysis. A dash means the bulletin sets no limit for that element.
Standards by product form
| Product form | Inconel 625 | Inconel 718 |
|---|---|---|
| Plate, sheet and strip | ASTM B443 / AMS 5599 / 5869 | ASTM B670 / B906 / AMS 5596 / 5597 |
| Rod and bar | ASTM B446 / B564 / AMS 5666 | ASTM B637 / AMS 5662 / 5663 / 5962 |
| Wire | ISO 9724 / AMS 5837 | AMS 5962 / 5832 / ISO 9724 |
| Pipe and tube | ASTM B444 | AMS 5589 / 5590 |
| Fittings | ASTM B366 | — |
The standard is written for the product form: quote the one that matches the product you are ordering. A dash means no standard is published for the grade in that form.
Forms, sizes and certificates for each grade are on the Inconel 625 and Inconel 718 pages. How 625 behaves in each acid, against the other grades, is in our acid and alkali service guide.